How to Read a Mist Eliminator Datasheet: The Six Parameters That Decide Performance
11/09/2026Why Demister Pads Collapse or Blow Out: Mechanical Failure Guide
11/09/2026Select the material from the corrosion environment first and the temperature second — never from habit. For neutral wet gas below about 400 °C, SS304 is adequate; for chlorides above roughly 50 ppm or any acid condensate, move to SS316L, Duplex 2205 or 6Mo; for wet chlorine, hypochlorite or hot concentrated acid, use Hastelloy C-276, PTFE, PVDF or PP. Temperature limits decide whether a polymer option is available at all.
Material decisions on mist eliminators go wrong in a specific way: the element is specified in SS316L because that is what the vessel is made of, and 18 months later the mesh is perforated while the vessel is still fine. The reason is that mesh has a far higher surface area to volume ratio than plate, and its thin wire is the first thing to lose. A material that survives as 10 mm plate does not automatically survive as 0.2 mm wire.
Service-based selection
| Service | Recommended | Avoid | Reason |
|---|---|---|---|
| Neutral wet gas, clean, < 400 °C | SS304 | Carbon steel | Adequate and economical |
| General chemical, mild chloride | SS316L | SS304 | Mo content resists pitting |
| Seawater scrubber wash water | SS316L, Duplex 2205, 6Mo | SS304 | Chloride pitting and crevice attack |
| Wet chlorine, hypochlorite | Hastelloy C-276, PTFE | SS316L, SS304 | Strong oxidiser attacks stainless |
| Sulphuric acid mist, concentrated | Hastelloy C-276, PTFE, glass fibre with PTFE cage | SS316L above ~70% concentration | Stainless corrodes in concentrated acid |
| Hydrochloric acid mist | PTFE, PVDF, Hastelloy C-276 | SS316L | Chloride attack even at low pH |
| Hot gas above 400 °C | SS321, SS316L, Inconel | Polymers | Polymer temperature limit |
| Caustic or alkaline wash | SS304, SS316L, Monel | Aluminium | Caustic stress corrosion |
| Amine or sour gas service | SS316L, Duplex | Carbon steel | Sulphide stress cracking |
Temperature limits by material
| Material | Practical continuous limit | Notes |
|---|---|---|
| PP | ~90 °C | Good general chemical resistance, low strength |
| PVDF | ~140 °C | Better temperature and strength than PP |
| PTFE | ~250 °C | Widest chemical resistance, low mechanical strength, needs support |
| SS304 / SS316L | ~400 °C continuous | Strength falls off above this; oxidation risk |
| Duplex 2205 | ~300 °C | Do not exceed; sigma phase formation |
| Hastelloy C-276 | ~600 °C | Broadest alloy resistance, highest cost |
| Borosilicate glass fibre (fiberbed) | ~180 °C | Media limit, not cage limit |
The wire-thickness trap
A demister mesh uses wire of 0.15–0.28 mm. At that thickness:
- Corrosion allowance is essentially zero — a loss of 0.05 mm removes a third of the section
- Pitting penetrates the full section almost immediately once initiated
- Erosion from entrained solids removes metal fast, especially at the top face
- Any galvanic couple with a larger cathode accelerates attack dramatically
This is why the material question on a mist eliminator is stricter than on the vessel. Where the vessel can be built in SS316L with a corrosion allowance, the mesh in the same service may need Duplex, 6Mo or Hastelloy.
Practical selection sequence
- Define the liquid chemistry: pH, chloride, oxidiser content, and any species known to attack stainless
- Define the temperature at the element, including excursion cases
- Decide whether a polymer is viable at that temperature; if yes, it usually wins on chemical resistance
- If a metal is required, choose the lowest grade that survives the chloride and acid environment — usually SS316L, then Duplex or 6Mo, then Hastelloy
- Check the support structure and fasteners in the same material; a SS316L mesh on a carbon steel support fails at the support
- Confirm that the selected material can be supplied at the required wire diameter — not every alloy is drawn to 0.15 mm
Our demister pads, fiberbed elements and plate pack media are available across these grades; send the service chemistry and we will confirm the grade and the wire diameter that can actually be produced.
Frequently Asked Questions
Which material should be used for a demister in seawater scrubber service?
SS316L is the standard choice for marine scrubber mist eliminators because the wash water is chlorinated and the temperature is moderate. Where chloride concentration or low pH pushes corrosion risk higher, Duplex 2205, 6Mo or a PP/PVDF alternative is used. Hastelloy is reserved for the most aggressive bleach or hypochlorite contact zones.
When is PTFE or PVDF preferable to a superalloy?
When the service is strongly oxidising or contains species that attack even high-nickel alloys at the operating temperature, and when mechanical strength is not the governing requirement. Polymer internals handle wet chlorine, hypochlorite and hot concentrated acids well, but they are temperature limited and need a rigid support structure.
Does material selection change the pressure drop?
Only indirectly. A change from metal mesh to a polymer mesh of the same density and thickness gives a similar dry pressure drop, but polymer components usually need a thicker wire for mechanical strength, which raises density and pressure drop for the same capture efficiency.
- Gas-Liquid Separation Fundamentals — terminology, separation mechanisms and internal selection
- Technical Data Sheet — material and performance reference data
- All Technical Articles — complete engineering index
If you are working on a replacement
Most of the work behind an article like this is a replacement inside an existing vessel, where the available dimensions decide more than the nominal duty. See the process data needed to size and select it, the scope from data review through to delivery and what has to be supplied before a price is issued.
More on wire mesh demisters and demister pads
- How Does a Wire Mesh Demister Work? A Complete Guide – the guide that covers this device family end to end
- Demister Sizing: Why Western and Chinese Conventions Give Different Diameters
- Why the Same Demister Duty Gives Different Diameters: Five Conventions That Move the Answer
- Reboiler Mist Eliminators in Ethylene, C3 Splitter Heat Pumps and Refrigeration Chillers